Product Knowledge

How is an on-site pull-out test on chemical anchors carried out? Sampling frequency and acceptance criteria explained

Views: 0Posted on: 2026-09-10

The short answer:On-site pull-out testing of chemical anchors is thelast line of defense, in accordance withJGJ 145-2013 Technical Specification for Post-Installed Anchoring of Concrete Structures. The sampling frequency is based onanchors of the same type, specification, and strength grade forming one inspection lot, with every1000 anchors forming one inspection lot, randomly select1‰ and no fewer than 5 anchorsfor testing. Acceptance is determined usingnon-destructive testing— apply1.2 times the design loadand hold for2 minutes, with a load drop of no more than5%, with no anchor slippage and no cracking of the substrate to be judged acceptable. Non-structural components of important structural members and lifeline projects require stricter sampling ratios. The load capacity of Daring chemical anchors at standard embedment depth often exceeds the design value by3-5 times, with the M12 pull-out force reachingover 60 kN, providing a generous safety margin for on-site testing.

In post-installed anchoring engineering, on-site pull-out testing of chemical anchors is thecore methodfor verifying whether anchoring quality meets design requirements. Many installers and supervisors lack a systematic understanding of sampling frequency, loading procedures, and acceptance criteria, leading to problems such as non-standard testing and inconsistent judgment criteria. This paper provides a comprehensive interpretation from the perspectives of sampling rules, loading methods, acceptance criteria, and failure mode analysis.

I. Sampling frequency: Inspection lot division and sample quantity

1.1 Principles for dividing inspection lots

According to JGJ 145-2013, when sampling for on-site inspection of anchoring quality,anchors of the same type, specification, and strength gradeinstalled in essentially the same anchoring locations onsimilar componentsshould constitute one inspection lot, and samples should be drawn from the anchors in each inspection lot.

The core of this principle is that only anchors with completely identical type, specification, and strength grade, and essentially the same anchoring locations (substrate conditions and stress states), can be grouped into the same inspection lot. Different areas and different substrate conditions (such as locations with differing concrete strength) should be sampled separately, avoiding sampling at structurally weak or repaired locations.

1.2 Sample quantity for non-destructive testing

Non-destructive testing is the most commonly used method on site, and its sample quantity is divided into three levels according to the importance of the structural component:

Component categorySample quantity
Important structural components and non-structural components of lifeline projectsWhen the total number of anchors in the inspection lot is ≤100, take20% and no fewer than 5 pieces; 10% when the total is 500; 7% when the total is 1000; 4% when the total is 2500; and 3% when the total is ≥5000. Values between two brackets may be determined by linear interpolation.
General structural componentsTake50% of the sample quantity for important structural components, with no fewer than 5 pieces
Non-structural components of non-lifeline projectsTake0.1% of the total number of anchors in each inspection lot and no fewer than 5 pieces

In actual engineering, curtain wall chemical anchors are usually grouped by every1000 anchors as one inspection lot, with fewer than 1000 anchors counted as one lot; from each lot,1‰ and no fewer than 5 anchors are randomly selectedfor pull-out testing.

1.3 Sample quantity for destructive testing

On-site destructive testing should preferably be carried out at locations with the same conditions outside the anchoring area, and should take0.1% of the total number of anchors in each inspection lot and no fewer than 5 piecesfor inspection. When the anchors are post-installed rebars and the quantity does not exceed 100 pieces,3 piecesmay be taken for inspection.

When any of the following conditions applies, destructive testing should be performed in addition to non-destructive testing:

  • Safety grade of Class Ipost-installed anchoring components

  • Cantilevered structures and components

  • Doubts about the post-installedanchoring design parameters

  • Doubts about theanchoring quality of the project

II. On-site pull-out test methods

2.1 Test equipment requirements

The loading equipment used for on-site testing may be a dedicated pull-out tester, which should comply with the following provisions:

  • The loading capacity of the equipment should beat least 20% greater than the expected test load value, and no more than 2.5 times the test load

  • The loading equipment should be capable ofcontinuous, smooth, and speed-controlledoperation.

  • For a hydraulic loading system, when the load-holding time does not exceed 5 minutes, itsload drop should not exceed 5%

  • The loading equipment should ensure that the applied tensile load is always aligned with theaxis of the post-installed anchoring component

Testing must be completed by a third-party testing agency possessingCMA certification, and a formal test report must be issued.

2.2 Loading methods

Loading may be carried out bycontinuous loadingorstepped loading, selected according to actual conditions:

  • Continuous loading: At a uniform rate, increase the load to the specified test load within2-3 minutes, and hold for2 minutes.

  • Stepped loading: Divide the specified test load into10 steps, with each step held for1 minute, until the specified test load is reached, then hold for2 minutes

With stepped loading, each of the first 8 steps is held for 1-1.5 minutes, and from the 9th step onward each step is held for 30 seconds, until the specified test load is reached, followed by a 2-minute hold.

2.3 Test timing requirements

For bonded anchors, testing should preferably be performed on the same day that the anchoring adhesive reaches thecuring time stated in the product data sheet.If sampling and testing must be postponed for any reason, in addition to obtaining the consent of the supervision unit,the postponement should not exceed 3 days. Testing of chemical anchors should be carried out after full curing, which usually takes ≥72 hours at normal temperature.

III. Acceptance criteria

3.1 Acceptance criteria for non-destructive testing

Acceptance in non-destructive testing requires the following conditions to be met:

  • Test load: Apply1.2 times the design load(1.3 times the design load for anchors)

  • Load-holding time: Hold for2 minutes

  • Load drop: The load drop during the 2-minute holdshould not exceed 5%

  • Visual behavior: No slippage, loosening, or abnormal noise of the anchors, and the substrate showsno cracking

Under standard installation, Daring chemical anchors can achieve a pull-out force of over 60 kN, and the test result should be anchor steel failure or concrete cone failure, rather than anchor pull-out.

3.2 Acceptance criteria for destructive testing

Destructive testing requires continuous loading until anchoring failure occurs, and the measuredultimate pull-out load capacityshould meet the design requirements. For post-installed rebars, the measured ultimate pull-out force should beno less than 1.45 times the design value。

3.3 Determination of failure modes

The determination of failure modes is the essence of test result analysis, directly revealing the weak links of the anchoring system:

Failure modeJudgmentDescription
Steel failure (anchor rupture)Ideal acceptable modeThe threaded rod is pulled apart while the anchoring adhesive and concrete remain intact, fully exploiting the material properties
Concrete cone failureAcceptable modeThe anchor is pulled out together with the surrounding cone-shaped concrete, occurring when the substrate strength is insufficient
Combined failureBorderline modePartial failure at the adhesive-concrete interface, requiring comprehensive judgment together with the measured load capacity
Anchor pull-outUnacceptableThe anchor is pulled directly out of the hole, indicating complete failure of the anchoring
Adhesive ruptureUnacceptableThe adhesive itself tears, indicating poor curing, deterioration, or installation defects

The ideal state issteel failure (anchor rupture)orconcrete cone failure; if anchor pull-out or adhesive rupture occurs, it is judged unacceptable.

IV. Handling of non-conformity and re-testing

4.1 Handling of non-conforming non-destructive test results

According to JGJ 145-2013, when non-destructive testing fails,at least 3 additional anchors should be sampled and subjected to destructive testingfor judgment. If destructive testing passes, the batch may continue to be used; if it still fails, the batch is judged non-compliant.

4.2 Handling of a single non-conforming piece

If a single anchor fails,double the sample size for re-testing. If re-testing still fails, the batch of anchors is judged not to meet the requirements and requiresrework or strengtheningtreatment. After rectification is completed, pull-out testing should be performed again, and work may proceed to the next process only when all results are acceptable.

V. FAQ

Q1What is the sampling frequency for on-site pull-out testing of chemical anchors?
Anchors of the same type, specification, and strength grade form one inspection lot. Important structural components are sampled at a ratio ranging from 20% (when ≤100 pieces) to 3% (when ≥5000 pieces); general components take 50% of the amount for important components and no fewer than 5 pieces; non-structural components of non-lifeline projects take 0.1% and no fewer than 5 pieces. Curtain wall projects usually treat every 1000 anchors as one inspection lot, from which 1‰ and no fewer than 5 anchors are selected.
Q2What are the acceptance criteria for non-destructive testing?
Apply 1.2 times the design load (1.3 times for anchors), hold for 2 minutes, with a load drop of no more than 5%, no slippage, loosening, or abnormal noise of the anchors, and no cracking of the substrate; the result is then judged acceptable.
Q3What is the ideal failure mode in a pull-out test?
The ideal state is steel failure (anchor rupture) or concrete cone failure. If anchor pull-out or adhesive rupture occurs, it is judged unacceptable, indicating weak links in the anchoring system.
Q4How should a failed pull-out test be handled?
When non-destructive testing fails, at least 3 additional anchors should be sampled for destructive testing. For a single non-conforming piece, the sample size should be doubled for re-testing; if re-testing still fails, the batch is judged non-compliant and requires rework or strengthening.
Q5What pull-out force can Daring chemical anchors achieve?
Daring M12 chemical anchors can achieve a pull-out force of over 60 kN, and their load capacity at standard embedment depth often exceeds the design value by 3-5 times. According to GB/T 3098.1-2010, the minimum tensile load of a class 8.8 M30 bolt reaches 466 kN, providing a generous safety margin for on-site pull-out testing.

The Daring chemical anchor series covers high-strength, capsule, reverse-cone, and dynamic-load reverse-cone anchors, paired with Daring's DL-200E modified epoxy injection anchoring adhesive, which meets the national Class A adhesive standard. Carbon steel of grade 5.8 or above, or 304/316 stainless steel, is available. Daring chemical anchors are manufactured strictly in accordance with JGJ 145-2013 and GB/T 3098.1-2010, with an M12 pull-out force of over 60 kN, providing a generous safety margin for on-site pull-out testing. For advice on on-site chemical anchor pull-out test plans for a specific project, please consult the Daring technical team.

References

JGJ 145-2013 Technical Specification for Post-Installed Anchoring of Concrete Structures - Appendix C: On-site Test Methods and Evaluation Criteria for Anchoring Load Capacity

GB 50550-2010 Code for Acceptance of Construction Quality of Strengthening Works of Building Structures - On-site inspection of anchor pull-out load capacity

GB 50210-2018 Standard for Acceptance of Construction Quality of Building Decoration - Inspection requirements for post-installed embedments in curtain wall works

JGJ/T 324-2014 Technical Specification for Testing of Building Curtain Wall Engineering - On-site pull-out test method for chemical anchors

Daring website - Chemical anchor product series

Daring website - Design values and testing standards for chemical anchor pull-out force

Back to Daring Home  Back to Top