First, the conclusion:Stainless steel back boltswill rust— "stainless" steel is not "rust-proof" but "rust-resistant." Under certain conditions, both 304 and 316 stainless steel back bolts can corrode, and among themintergranular corrosionandstress corrosion cracking (SCC)are the two most insidious and dangerous failure modes. Intergranular corrosion stems from thesensitization (450–850°C), chromium carbides precipitate at grain boundaries, forming chromium-depleted zones and leading to preferential grain-boundary corrosion. Stress corrosion cracking, on the other hand, istensile stress + chloride ions + sensitization temperaturethe combined effect of the three factors. The risk is extremely high in coastal high-salt-spray, industrial-pollution, and wet-dry cycling environments. Daring back bolts are made of 304/316 stainless steel, among which the S316 material (containing 2%-3% molybdenum) has a pitting resistance equivalent number PREN≥24, and its resistance to intergranular corrosion and stress corrosion cracking is significantly better than that of 304. For coastal projects, chemical environments, and projects involving welding operations,316 (A4) stainless steel back bolts must be used。
In curtain wall engineering, back bolts are exposed to outdoor environments for extended periods, subjected to the combined effects of wind loads, temperature changes, and corrosive media. Many engineers believe that "stainless steel does not rust," which is a serious misconception. Starting from corrosion mechanisms, this paper systematically analyzes the risks of intergranular corrosion and stress corrosion cracking in stainless steel back bolts, helping engineers select materials scientifically and avoid hidden dangers.
I. Why stainless steel "rusts"
1.1 Anti-corrosion principles of stainless steel
The corrosion resistance of stainless steel derives from an extremely thinchromium oxide passive film(Cr₂O₃), only a few nanometers thick but extremely dense, which effectively prevents oxygen and corrosive media from contacting the base metal. When the passive film is intact, stainless steel has good corrosion resistance; once the passive film is damaged and cannot repair itself, corrosion occurs.
Stainless steel screws have an oxide film on their surface. If it is damaged by impact or collision and the surface is breached, then in a humid environment or in the presence of impurities, rapid rusting will occur. Deposits of dust or metal particles in humid air form micro-cells with the condensed water on the stainless steel surface, triggeringelectrochemical corrosion, damaging the protective film.
1.2 Common types of stainless steel corrosion
Stainless steel corrosion can be classified asuniform corrosion, pitting, crevice corrosion, intergranular corrosion, and stress corrosion crackingand other types. Among them,intergranular corrosion and stress corrosion crackingbecause of their insidious nature and great destructiveness, are thetwo failure modes that require the greatest vigilance in back bolt applications。
II. Intergranular corrosion: Invisible "internal friction" at grain boundaries
2.1 Mechanism of intergranular corrosion
Intergranular corrosion is a form of localized corrosion that occurs along the grain boundaries of metals. Its root cause lies insensitization— when stainless steel is heated in the450-850℃temperature range (i.e., the sensitization temperature zone), the carbon at the grain boundaries combines with chromium to formchromium carbide (Cr₂₃C₆), causing the chromium content near the grain boundaries to decrease and formingchromium-depleted zones。
In solution-annealed austenitic steel, carbon is dissolved in the austenite in a supersaturated state, but this is not a stable state. When the metal is subjected to sensitization temperatures, the supersaturated carbon diffuses toward the grain boundaries and forms Cr₂₃C₆ precipitates there. The chromium content of the chromium-depleted zones is insufficient to form a dense passive film, so they are preferentially corroded in corrosive media, causing loss of bonding force between grains.
2.2 Risk scenarios for intergranular corrosion in back bolt applications
During the production and installation of back bolts, the following situations may induce intergranular corrosion:
Welding heat effects: During welding of back bolts to pendants or angle brackets, the heat-affected zone reaches sensitization temperatures and chromium carbides precipitate at the grain boundaries. Repeated heating in multi-pass welding causes the weld metal to remain in the sensitization temperature range for a longer time, aggravating the tendency toward intergranular corrosion.
Improper heat treatment: If temperature and time are not strictly controlled during heat treatment in back bolt production, the product may enter a sensitized state.
Corrosive media environments: In coastal high-salt-spray areas, industrially polluted zones, and acidic or alkaline media environments, the grain boundary corrosion rate of sensitized stainless steel is significantly accelerated.
2.3 How to prevent intergranular corrosion
Select steels containing stabilizing elements: Adding titanium (Ti) or niobium (Nb) preferentially combines with carbon, avoiding consumption of chromium.
Reduce carbon content: Ultra-low-carbon stainless steels such as 316L (C≤0.03%) effectively prevent intergranular corrosion.
Control the welding process: Reduce welding heat input, avoid repeated heating in multi-pass welding, and shorten the dwell time in the sensitization temperature range.
Select welding materials resistant to intergranular corrosion。
Solution treatment: Reheat the sensitized stainless steel to above 1050°C and cool rapidly to redissolve the chromium carbide.
III. Stress corrosion cracking (SCC): The most dangerous failure mode
3.1 Mechanism of stress corrosion cracking
Stress corrosion cracking (SCC) is the most common failure mode of austenitic stainless steels, especially the commonly used304 and 316 stainless steels. Its occurrence requires three conditions to be met simultaneously:
Tensile stress: including working stress and residual stress (such as stress from cold working, welding, and installation)
Corrosive media: in particular,chloride ion (Cl⁻)environments
Sensitization temperature: a history of thermal exposure at 450-850°C
The mechanism of chloride stress corrosion cracking is: after the passive film is breached by chloride ions, pits form through an "autocatalytic process," and cracks propagate along grain boundaries or through grains under stress.Wet-dry cyclingis an important factor in inducing pitting and chloride stress corrosion cracking.
3.2 Risk scenarios for SCC in back bolt applications
Coastal curtain wall projects: Sea breezes carry large amounts of chloride ions, and wet-dry cycling is frequent, making these high-incidence areas for SCC.
Industrially polluted areas: The atmosphere contains corrosive media such as chlorides and sulfides.
Back bolts that have been welded or cold-worked: Welding residual stress and cold-working stress provide the stress conditions for SCC.
Back bolts subjected to cyclic loads over the long term: Cyclic stresses from wind loads and temperature changes accelerate crack propagation.
3.3 How to prevent stress corrosion cracking
Select 316/316L stainless steel: Adding 2%-3% molybdenum (Mo) significantly improves resistance to chloride corrosion.
Eliminate residual stress: Remove welding and cold-working stresses through heat treatment or mechanical methods.
Avoid wet-dry cycling environments: Take effective drainage and ventilation measures.
Control chloride ion concentration: In corrosive environments, clean the surface regularly to reduce chloride deposition.
IV. 304 vs 316: Comparison of corrosion resistance
4.1 Differences in chemical composition
| Comparison item | 304 stainless steel (A2) | 316 stainless steel (A4) |
|---|---|---|
| Chromium (Cr) content | 18%-20% | 16%-18% |
| Nickel (Ni) content | 8%-10% | 10%-14% |
| Molybdenum (Mo) content | — | 2%-3% |
| Pitting Resistance Equivalent Number (PREN) | 18-20 | ≥24 |
4.2 Comparison of salt spray test data
According to NSS neutral salt spray test data:
304 stainless steel: approximately303 hoursred rust appears
316 stainless steel: approximately550 hoursred rust appears
The corrosion resistance of 316 stainless steel is approximately1.8 times that of 304The molybdenum added to 316 stainless steel makes its seawater corrosion resistance significantly better than that of 304, with a pitting resistance equivalent number (PREN) of ≥24. Even after thousands of hours of salt spray testing, the passive film of 316 stainless steel remains intact.
4.3 Intergranular corrosion and SCC performance comparison
Because 316 stainless steel contains molybdenum, itsintergranular corrosion resistanceis superior to that of 304 stainless steel. Lowering the carbon content also better prevents intergranular corrosion. fischer back bolts are made of A4 (316L) stainless steel, which offers particularly high resistance to marine and aggressive industrial atmospheres as well as high-temperature strength, and can be used under severe conditions, with excellent intergranular corrosion resistance.
V. Decision guide for selecting back bolt stainless steel
5.1 Selection recommendations for different environments
| Environment type | Recommended material | Risk warning |
|---|---|---|
| General indoor environments | 304 stainless steel (A2) | Low risk |
| General outdoor/inland environments | 304 stainless steel (A2) | Avoid welding heat effects |
| Coastal areas (within ≤5 km of the sea) | 316 stainless steel (A4) | High salt spray + wet-dry cycling → SCC risk |
| Industrial pollution/chemical environments | 316 stainless steel (A4) | Chloride ions/sulfides accelerate corrosion |
| Back bolts with welding operations | 316L stainless steel | Ultra-low carbon + molybdenum resist intergranular corrosion |
5.2 Core selection principles
Coastal high-salt-spray environments:316 (A4) stainless steel must be usedCodes require back bolts to be made of austenitic stainless steel no lower than 06Cr17Ni12Mo2 (S31608), and 316 stainless steel is recommended as the preferred material to ensure long-term durability.
With welding operations: Select 316L (ultra-low-carbon) stainless steel, to avoid sensitization in the welding heat-affected zone.
General inland environments: 304 stainless steel is cost-effective, but attention must be paid to protecting the surface passive film.
Avoid electrochemical corrosion: The materials of back bolts, pendants, and connecting bolts should be matched to avoid galvanic corrosion between dissimilar metals.
VI. FAQ
| Q1 | Do stainless steel back bolts rust? Yes. "Stainless" steel is not "rust-proof" but "rust-resistant." When the surface passive film is damaged (e.g., by scratches, impact, or welding heat effects), stainless steel will still corrode in humid or corrosive environments. |
| Q2 | What is the difference between intergranular corrosion and stress corrosion cracking? Intergranular corrosion occurs along grain boundaries and stems from chromium-depleted zones caused by sensitization; stress corrosion cracking results from the combined action of tensile stress + chloride ions + sensitization temperatures. Both can occur in back bolts, but SCC is more insidious and more destructive. |
| Q3 | Which is more durable, 304 or 316 stainless steel back bolts? 316 is more durable. 316 contains 2%-3% molybdenum, has a pitting resistance equivalent number PREN≥24, and its time to red rust in salt spray testing (550 hours) is about 1.8 times that of 304 (303 hours). 316 must be used in coastal and corrosive environments. |
| Q4 | Does welding affect the corrosion resistance of back bolts? Yes. If the welding heat-affected zone reaches sensitization temperatures (450-850°C), chromium carbide precipitates and forms chromium-depleted zones, reducing intergranular corrosion resistance. 316L ultra-low-carbon stainless steel should be used, and the welding process should be controlled. |
| Q5 | What stainless steel does Daring use for its back bolts? The Daring back bolt series covers hammer-in, screw-in, cast-in, and high-load back bolts, made of 304/316 stainless steel. Among them, back bolts made of S316 material offer better corrosion resistance and are suitable for coastal and corrosive environments. |
The Daring back bolt series covers hammer-in, screw-in, cast-in, and high-load back bolts, made of 304/316 stainless steel, achieving stress-free dry-hung anchoring of exterior wall panels through mechanical locking. Daring back bolts are available in A2 (304) and A4 (316) stainless steel, with S316 material offering better corrosion resistance. For back bolt stainless steel selection advice for a specific project, please consult the Daring technical team.
References
Daring website - Back bolt product series
Daring website - What tests should be performed before back bolts are installed on walls
GB/T 4334-2008 Corrosion of Metals and Alloys - Test Methods for Intergranular Corrosion of Stainless Steels
GB/T 20801.1-2025 Code for Pressure Piping - Industrial Piping - Part 1: General - Chloride stress corrosion cracking
ASTM G48 Standard Test Methods for Pitting and Crevice Corrosion Resistance of Stainless Steels and Related Alloys by Use of Ferric Chloride Solution
General technical literature on stainless steel corrosion - Mechanisms of intergranular corrosion and stress corrosion cracking